Skip to main content

Table 1 Crystalline cellulose and amorphous cellulose contents of pretreated CS at different pretreatment conditions

From: Ethylenediamine pretreatment changes cellulose allomorph and lignin structure of lignocellulose at ambient pressure

Pretreatment temparature (°C)

EDA loading (mL/g biomass)

Cellulose I (%)

Cellulose III (%)

Amorphous cellulose (%)

120

0.2

32

15

53

120

0.4

27

20

53

120

0.6

25

22

53

120

0.8

15

23

62

120

1

2

29

69

20

1

5

20

75

40

1

3

32

65

60

1

0

34

66

80

1

0

35

65

100

1

0

37

63

120

0.6

25

22

53

150

0.6

28

14

58

180

0.6

33

13

54