Sample | Component recovery in LHW liquid fraction (% of total component amount) | Component recovery in LHW solid fractions (% of total component amount) | Weight loss (DW %) | |||||
---|---|---|---|---|---|---|---|---|
Cellulose | Hemicellulose | Sugar transformation by-products | Cellulose | Hemicellulose | Acid-soluble lignin | Total lignin | ||
TS-120 | 42.0 ± 4.4 | 0 | 5.7 ± 0.5 | 69.8 ± 1.2 | 90.2 ± 3.7 | 90.7 ± 1.8 | 81.9 ± 3.2 | 20.9 ± 1.9 |
TS-160 | 51.3 ± 2.3 | 1.5 ± 0.2 | 6.9 ± 0.7 | 75.9 ± 2.6 | 81.6 ± 2.8 | 68.2 ± 5.2 | 80.3 ± 1.7 | 32.1 ± 2.5 |
TS-200 | 15.5 ± 3.8 | 0 | 11.9 ± 0.8 | 65.4 ± 3.4 | 28.4 ± 3.3 | 26.7 ± 3.6 | 67.6 ± 2.2 | 56.9 ± 0.8 |
PT-TS-120 | 0 | 0.5 ± 0.04 | 2.4 ± 0.3 | 59.5 ± 2.1 | 81.5 ± 0.9 | 33.9 ± 0.9 | 31.9 ± 4.1 | 12.5 ± 0.7 |
PT-TS-160 | 4.9 ± 0.7 | 0.5 ± 0.03 | 2.3 ± 0.2 | 58.8 ± 3.5 | 69.2 ± 2.1 | 24.7 ± 2.9 | 28.7 ± 2.6 | 24.4 ± 1.2 |
PT-TS-200 | 11.3 ± 1.6 | 0 | 5.7 ± 0.5 | 58.2 ± 4.3 | 59.6 ± 3.0 | 8.8 ± 3.4 | 32.4 ± 2.0 | 34.6 ± 1.6 |